1. Klas Materyèl Prensipal

Q:Ki klas asye yo estanda pou tib affine?
A:

Asye kabòn:

ASTM A519 1020/1026 (σᵧ Pi gran pase oswa egal a 350 MPa, itilizasyon idwolik jeneral).

DIN 2391 St52 (Almay), JIS G3445 STKM 13A (Japon).

Asye alyaj:

4130/4140 (Cr-Mo, pou gwo - silenn presyon, dite 200-250 HB).

Nerjaveèi asye:

304/316 (ASTM A312) pou aplikasyon koroziv oswa manje-.

Nòt:CK45 (DIN) se yon ekivalan komen Ewopeyen an 1045 (ASTM).


2. Kontwòl Konpozisyon Chimik

Q:Ki limit konpozisyon kritik?
A:

Eleman Limit (poids%) Enpak
C 0.18–0.28 Fòs/perfectionner konpatibilite
S/P Mwens pase oswa egal a 0.025 Anpeche mikwo-fann
Kr 0.8–1.1 (4130) Amelyore hardenability
Kle:Ba O/N/H (mwens pase oswa egal a 30 ppm) pou fè pou evite porosite pandan perfectionnement.    

3. Kondisyon pou tretman chalè

Q:Ki jan tib afè yo trete tèmikman?
A:

Nòmalizasyon:900-950 degre (ASTM A519) pou estrikti grenn inifòm.

Trempe & Tanperaman (Q&T):Pou 4140: 850 degre lwil oliv pasè → 600 degre tanperaman.

Soulaje estrès:Post-perfectionnement nan 500-550 degre (ISO 10763).
Rezilta:σᵧ 550-850 MPa ak 15-20% elongasyon.


4. Sifas Fini & Honing Standards

Q:Poukisa sifas fini kritik?
A:

Personaj klas:Ra Mwens pase oswa egal a 0.4 µm (ISO 1219) pou sele U-cup/piston.

Opsyon plating:

Kwòm difisil (20-50 µm, ISO 4525).

Electroless nikèl (pou rezistans korozyon).

Polisaj:Fini glas (Ra mwens pase oswa egal a 0.2 µm) pou aplikasyon pou gwo vitès-.
Tandans 2025:Lazè-pwosesis ibrid perfectionnement reyalize Ra Mwens pase oswa egal a 0.1 µm.


5. Validasyon Kalite & Sètifikasyon

Q:Ki jan yo verifye entegrite materyèl?
A:

NDT:100% ultrasons (ISO 10893-1) + tès aktyèl eddy.

Tès mekanik:Tensile (ASTM E8), enpak Charpy (ISO 148-1).

Sètifikasyon:ISO 10763 (idwolik), DIN 2391 (presizyon), PED 2014/68/EU (ekipman presyon).